Request a Metal Injection Molding Quote

Share your drawing, material requirements, annual volume, tolerance needs, or application details. Our engineering team will review your MIM project and respond with technical feedback or a quotation.

MIM Holes Slots Undercuts Design Guide

MIM DESIGN & ENGINEERING

MIM Holes, Slots and Undercuts Design Guide

Designing holes, slots and undercuts for Metal Injection Molding (MIM) requires careful consideration of feature geometry, mold opening direction, core pin support, tooling complexity and sintering behavior. Learn how to design manufacturable features, reduce flash and distortion risks, meet functional tolerances, and determine when direct molding, secondary machining or design modifications offer a more reliable and cost-effective manufacturing solution.

Key Design Considerations

MIM can directly form through holes, blind holes, slots and many external undercuts. Features aligned with the mold opening direction are generally easier to produce, while deep blind holes, narrow slots and internal undercuts require closer evaluation of core pin support, tooling strength, mold release and sintering stability.

Design Priorities

  • Align holes and slots with the mold opening direction where function permits.
  • Maintain sufficient material around holes and slots.
  • Verify core pin support and undercut release paths.
  • Evaluate long slots for sintering distortion.
  • Reserve secondary machining for features that cannot reliably meet functional requirements through direct molding, where machining access and allowance permit.

For the wider design process, consult the MIM Design Guide. Related design considerations include MIM part design, MIM wall thickness design, MIM mold design and MIM tolerances.

What Holes, Slots and Undercuts Can MIM Produce?

MIM is particularly useful when holes, slots and retaining features can be integrated into a small metal component rather than added by separate machining or assembly. Coring can also remove excess material from thick sections. The initial risk classification depends on the actual dimensions and function of each feature; it does not establish production capability.

Feature MIM Suitability Main Design Risk DFM Review Focus
Through holes Usually suitable Core pin deflection, flash, hole distortion Hole direction, depth, diameter and tolerance
Blind holes Possible but more sensitive Unsupported core pin, trapped geometry, ejection risk Depth-to-diameter ratio and core pin support
Side holes Possible with tooling review Slides, side actions, parting line flash Mold motion and shutoff surface
Narrow slots Conditional on tool and part geometry Filling difficulty, flash, weak tool steel Slot width, depth and edge condition
Long slots Risk-sensitive Sintering distortion, wall imbalance Wall thickness, support and shrinkage path
External undercuts Conditional on release direction Slide action, parting line mark, flash Ejection direction and split line
Internal undercuts High-risk Complex tooling, collapsible core, flash Redesign, split feature or secondary operation

A feature should be assessed in its proposed mold orientation. A hole or groove that looks difficult from one direction may become straightforward when the parting plane changes. Conversely, a small feature can become a major risk if it lies on a sealing face or requires a slender unsupported core.

What Determines Feature Manufacturability in MIM?

Feature Orientation, Parting Lines and Mold Release

Establish a candidate mold opening direction and trace the withdrawal path of every core and cavity member. A feature aligned with that path may be formed in a straight-pull tool; a transverse feature may need a split cavity or side action. Identify where the steel-to-steel shutoff and witness lines will lie. Mark any sealing, sliding or cosmetic surfaces where flash or mismatch would be unacceptable.

Core Support and Tooling Strength

A core pin forms a hole; a projecting insert or blade may form a slot. A slender pin supported at one end behaves like a cantilever, so asymmetric feedstock pressure can displace it. Supporting the opposite end or shortening the unsupported span can improve stability. A narrow, deep slot can similarly leave a weak steel projection in the mold. Tool steel thickness, access for replacement and wear at shutoffs matter alongside the nominal part dimensions.

Local Geometry and MIM Process Behavior

Flow splits around cores and rejoins downstream. The remaining metal sections must be thick enough for filling and handling, yet not so uneven that binder removal and shrinkage become difficult to control. Evaluate the green part, the debound part and the sintered part as separate states. A geometrically correct green part can still distort during densification. See MIM mold design for the complete tooling review.

How to Design Holes for Metal Injection Molding

First identify whether the hole is for clearance, weight reduction, alignment, fastening or a precision fit. The hole function determines which geometric changes are acceptable.

Through Holes and Blind Holes

A through hole allows a core to be supported at both ends in suitable tooling. A blind hole usually needs a projecting core with no support at its tip. Where the function permits, convert a deep blind hole to a through hole, reduce its depth or increase its diameter. Preserve adequate material at the blind end and avoid abrupt changes in section. For a flat-bottomed functional recess, specify the usable depth and permitted corner radius rather than assuming a perfectly sharp bottom.

Side Holes and Intersecting Holes

A side hole is transverse to the chosen opening direction, not necessarily horizontal in the drawing. Consider rotating the mold orientation or placing the feature on a practical split before adding a slide. Intersecting holes formed by separate cores may require a reliable steel-to-steel shutoff where the cores meet. A circular intersection can leave delicate steel edges at the contact. If flow area and fit allow, a D-shaped cross hole provides a flat shutoff surface; this is a design option, not a substitute for checking the mating core geometry. See the MIMA complex design guide.

Hole Diameter, Depth and Spacing Guidelines

For two neighboring round holes, the nominal remaining ligament is center spacing minus half the sum of their diameters. For a round hole beside a straight edge, it is the perpendicular center-to-edge distance minus half the diameter. Check the worst-case ligament after positional and size tolerances, not just the nominal CAD value. The required ligament depends on loading, filling and the surrounding geometry.

For a tapered hole, specify the minimum usable diameter over the required engagement length rather than only the entry diameter. For a straight conical bore, the diameter difference over depth L is 2L × tan(draft angle), assuming draft is measured from the axis on each side. This geometric relationship is not a process tolerance. Use the following values as early screening references, not drawing acceptance limits. For preliminary drawing screening, use the nominal finished hole depth and diameter. For tool design, calculate the actual core diameter and unsupported span separately, allowing for shrinkage, taper and the support arrangement.

Design variableScreening guidanceWhat to verify
Minimum hole diameterPIM International advises avoiding holes below 0.1 mm. This is not a generally achievable minimum.Powder/feedstock, pin strength, depth, inspection and supplier trial.
Blind hole depthEPMA suggests a general depth of about 2 times core diameter.Core deflection, pressure balance, release and bottom thickness.
Through vs. blind hole selectionMIMA favors through holes over blind holes above L/D = 4:1. This is a preference, not a maximum through-hole ratio.End support, straightness and position.
DraftMIMA and EPMA give 0.5 to 2 degrees where taper is required.Usable diameter along depth and permitted taper.
Edge distance and pitchNo universal feature spacing is assumed.Remaining ligament, mold steel, load and flow path.

For example, a 1 mm diameter blind hole 4 mm deep has a nominal depth-to-diameter ratio of 4:1. It warrants explicit core support review rather than automatic approval or rejection. The ratio does not establish a manufacturing tolerance.

References: EPMA MIM design guidance and PIM International design recommendations.

How to Design Slots and Grooves for MIM Parts

Open Slots, Closed Slots and Recessed Grooves

Open-ended slots interrupt an external edge. Closed slots are surrounded by material in plan view, while recessed grooves have a remaining floor. A practical withdrawal path is necessary for direct molding, but tool strength, filling, release and final dimensions must also be verified. An open slot is not automatically easier: depth, orientation and the support of its forming insert still matter. Define whether the slot guides a moving part, provides clearance or retains a component.

Slot Width, Depth, Length and Corner Design

ParameterDesign checkPossible improvement
Width and depthCheck the thickness and unsupported height of the forming blade.Widen or reduce depth where function permits.
LengthCheck the remaining rails and bridges for stiffness.Shorten or relocate the slot, or reinforce the remaining section.
End radiusCheck sharp internal corners and machining access.Use the largest functional radius permitted by the mating part.
Edge distance and spacingCheck remaining metal and tool steel between nearby features.Move features or redistribute material without abrupt section changes.

A practical minimum slot width and depth-to-width ratio depend on the forming blade and part geometry. A dimension that is practical in a shallow open slot may be unsuitable in a deep enclosed slot. Do not apply blind-hole ratios to slot blades. Consult wall thickness design when the remaining section is the limiting condition.

Designing Stable Long and Narrow Slots

Check the minimum usable slot width along the full engagement length. For a straight tab and slot, the preliminary worst-case total width clearance is the smallest permitted slot width minus the largest permitted tab width. For example, a 2.00 ± 0.05 mm slot and a 1.90 ± 0.03 mm tab leave 0.02 mm nominal worst-case total clearance before any additional inward flash, coating build-up or misalignment not already included in the final dimensions. These example dimensions illustrate the clearance calculation, not achievable MIM tolerances. Verify straightness, datum alignment and the required running clearance separately. A wider slot may strengthen its forming blade but simultaneously weaken the remaining metal rails, so widening is not always an improvement.

Examine the two rails beside a long slot as structural members. A slot close to one edge can leave a slender rail that responds differently during handling and sintering. Where function allows, balance the remaining sections and provide gradual transitions. Review whether a flat setter can support the component without preventing shrinkage; dedicated support may be needed for long spans. Verify slot width at multiple locations rather than only at the center.

XTMIM sintering furnace during part loading
Part loading at the XTMIM sintering furnace.

When reviewing long slots or thin bridges, confirm the proposed part orientation, support contact areas and freedom to shrink during sintering. This factory photograph provides loading context; it does not demonstrate a validated support arrangement for a particular slot geometry.

How to Design Undercuts for MIM Parts

External and Internal Undercuts

In an engineering drawing, an undercut is a region that obstructs withdrawal along the proposed tool direction. External retaining grooves, hooks and recesses may be accessible to a split cavity; an internal annular groove inside a bore can trap a rigid core. The distinction depends on the intended tooling movement, not simply the appearance of the CAD model. Closed internal cavities and hidden internal undercuts deserve particular scrutiny.

Undercut Geometry and Mold Release Options

Check the depth and position of the feature, the space available for side movement and the order in which mold members must withdraw. For an annular internal groove, compare the largest diameter of the rigid forming core with the smallest bore opening along its exit path. If the core cannot pass through that opening, a straight axial pull cannot release it. A retractable core must fit through the opening in its contracted state with practical clearance; its availability and strength must still be confirmed. A split cavity may create witness lines across an external retaining groove; if that groove seals against an O-ring, flash and mismatch need explicit limits. Some internal forms can be made using side actions or collapsible cores, but small MIM components may leave insufficient room for such mechanisms. Do not rely on elastic stripping of a fragile green part without validation. EPMA notes that collapsible cores are often impractical for small MIM parts; hidden internal undercuts should therefore be treated as a redesign or machining candidate unless a feasible tooling route is demonstrated.

Design Alternatives for Difficult Undercuts

Original featurePossible alternativeFunction to preserve
Hidden internal retaining grooveOpen the access path or evaluate internal grooving after sintering.Retention and mating clearance.
External hook blocking releaseChange the split or hook orientation.Load-bearing face and engagement.
Multiple opposing recessesAlign withdrawal directions where feasible.Assembly and location.
Non-critical reliefSimplify or remove it with design approval.Required clearance.

A redesign is successful only if the revised geometry performs the same required function. Check the mating component, load direction and permitted assembly sequence before removing or relocating an undercut.

How Feature Design Affects MIM Defects and Production Stability

Tooling, Filling and Green-Part Failure Risks

Use the first stage at which a defect is observed to guide investigation. Compare the green component with the final sintered component before attributing a dimensional problem to the mold. Compare shape and location relative to equivalent datums after allowing for expected shrinkage; raw green and sintered dimensions are not directly comparable. If a shift consistently follows one cavity, inspect that cavity and its core first; if the green geometry is sound but the normalized shape changes after sintering, investigate handling, support and thermal processing. Neither observation proves a single root cause.

Stage and symptomPossible causeDiagnostic or prevention check
Injection: hole shiftSlender core deflection or mismatchCompare green hole position across cavities; review core support.
Injection: flash around side holeShutoff wear, mismatch or local pressureInspect tool contact and flash location; protect functional surfaces.
Injection: short shot or knit lineFlow around core, restricted section or trapped airReview gate design and venting.
Ejection: crack or bent railInterference or uneven release loadInspect green parts and review draft and ejector support.
Debinding: crackingSection imbalance or binder removal conditionsCheck thickness and process history.
Sintering: slot distortionWeak rail, support or nonuniform densificationCompare pre/post-sinter dimensions and setter contact.

Example: Flash Around a Side Hole

Potential failure
Consider a small MIM housing with a side hole near a cosmetic surface. Flash around the opening could require extra removal and affect appearance.
Likely factors to investigate
If the hole requires a slide, limited shutoff support or imperfect contact near the visible surface could allow feedstock to escape. Tool fit and process conditions would need inspection.
Design implication
A flash-sensitive interface may conflict with the protected cosmetic surface.
Design options
Evaluate moving the hole or relieving a non-functional surface to improve the shutoff; identify acceptable mark zones on the drawing and verify the revised tool during trials.
Pre-tooling check
Side holes should be reviewed with parting line, slide direction, shutoff condition and surface classification before tooling approval.

Debinding, Sintering and Dimensional Distortion Risks

A hole can reduce a thick section, but abrupt changes around the hole may complicate binder removal. A long slot can leave a weak frame that distorts after molding. Debound parts are particularly vulnerable during handling. During sintering, evaluate support and shrinkage together; changing the mold scale alone will not correct every local distortion. See sintering support design.

Example: Long Slot Distortion After Sintering

Potential failure
Consider a thin MIM part with a long narrow slot near one edge. Its green geometry may appear acceptable while the sintered slot becomes bowed or varies in width.
Likely factors to investigate
Unequal remaining sections and setter contact may allow the rails to move differently during sintering. Compare the part before and after sintering to distinguish this from molding or handling distortion.
Design implication
The clearance slot also determines the stiffness and section balance of the remaining frame.
Design options
Evaluate a more balanced slot position, gradual wall transitions and a suitable setter orientation. An increased end radius may help local stress but does not alone establish dimensional stability.
Pre-tooling check
Long slots should be checked together with wall thickness, shrinkage path and sintering support before tooling is finalized.

Both examples describe hypothetical design conditions, not measured production results.

How to Meet Functional and Dimensional Requirements in MIM Features

Define Functional Dimensions and Critical Tolerances

A clearance hole and a locating bore can have the same nominal diameter but very different acceptance requirements. Specify the final functional dimension, datum relationship, fit, permitted flash and surface condition on the drawing. For a guide slot, specify whether width, straightness or parallelism controls motion. For a retaining groove, identify the engagement surfaces and the mating component. Do not tighten every non-critical dimension to the same level.

As-Sintered Accuracy, Inspection and Repeatability

Agree whether each dimension applies to the as-sintered or finished condition. EPMA gives a general dimensional reference of ±0.3% (±0.003 mm/mm). This is a starting point for dimensional planning, not a guaranteed tolerance for small holes, slot form or true position. Local geometry, shrinkage and measurement uncertainty require separate validation. See MIM tolerances for broader tolerance planning.

Feature Area Typical Inspection Focus Possible Check Method Why It Matters
Through holes Diameter, position, roundness and blockage Pin gauge, optical measurement or CMM based on tolerance requirement Assembly pins, fasteners or shafts may fail if the hole shifts or shrinks unevenly.
Blind holes Depth, bottom condition and usable entry Depth gauge, optical inspection or section review when required Unsupported core pins and trapped geometry can create variation or incomplete functional depth.
Side holes and undercuts Flash, parting line marks, shutoff wear and opening condition Visual inspection, magnification, go/no-go gauge or functional fit check Slide and shutoff areas can create flash that affects assembly, sealing or appearance.
Long slots Slot width, straightness, parallelism and local distortion Optical measurement, fixture check or CMM for critical dimensions Slots may distort during sintering even when green part molding looks acceptable.
Cosmetic or sealing surfaces near features Witness lines, burrs, flash removal marks and surface interruption Visual standard, surface comparison or application-specific inspection Feature location can move tooling marks onto surfaces that buyers expect to remain clean.
Critical mating features Functional fit, alignment and repeatability Assembly fixture, go/no-go gauge or defined dimensional inspection Functional dimensions should be identified before RFQ so molded and machined tolerances are not confused.

A pin gauge can check passage or limit size but does not independently establish hole position or roundness. Use suitable datum-based measurement when location controls assembly. Confirm gauge access and repeatability before tooling. For a multi-cavity tool, record cavity identity and compare results across cavities and representative production lots. For a critical slot, record the minimum usable width and the locations of measurements, not just an average. Agree the acceptance method before claiming process capability; a single conforming sample does not establish repeatability.

When to Mold, Machine or Redesign MIM Features

Direct Molding and Special Tooling Solutions

Select straight-pull molding for features with a clear release path and acceptable as-sintered requirements. Consider slides or split cavities when a required feature cannot be released conventionally and the added mechanism removes meaningful downstream work. Confirm the tool motion, shutoff location and maintenance plan before choosing.

When Secondary Machining Is More Suitable

Consider post-sintering machining when a critical bore, slot or retaining form cannot reliably meet the drawing in the molded condition and the machining route is itself feasible. Drilling, reaming, milling or tapping may be suitable if the feature is accessible and can be located from stable datums. A pilot feature may be molded with stock for finishing. For a round pilot bore, the nominal radial stock is half the difference between the finished and pilot diameters. Check the largest expected sintered pilot diameter and its offset from the intended finished axis: a pilot that already extends outside the final bore envelope may leave an uncut surface even when nominal stock appears adequate. Also check remaining wall thickness after finishing, fixture access and datum stability. Sizing is another option for compatible geometries but cannot correct every form or location error. See post-sintering machining.

When Feature Redesign Is the Better Solution

Prefer a design change when tooling and machining both create excessive risk or when a non-critical feature adds cost without functional benefit. Reorient a hole, shorten a slot or open a trapped groove only after checking the mating geometry and obtaining design approval.

RouteSuitable whenConfirm before release
Direct moldingClear release path and adequate as-sintered capabilityCore support, dimensions and inspection.
Special toolingEssential side feature with practical motionShutoff, wear, flash and volume.
Secondary machining or sizingFunctional accuracy or difficult molded featureAccess, stock, datum, material and cost.
RedesignFeature can be changed without compromising functionMating part, load and customer approval.

Example of a combined manufacturing route: A compact bracket has a clearance through hole, a precision transverse locating bore, a long guide slot and an internal retaining groove. Mold the clearance hole if core support is adequate; evaluate datum-based drilling or boring to establish location, followed by reaming if required for size and finish; check slot rail stability and final straightness; and compare a revised accessible retention feature with machining the original groove. These choices can coexist in one manufacturing route.

How Feature Design Affects Tooling and Part Cost

Compare incremental costs for the same accepted part, not simply mold quotations. A side action adds fixed tooling investment and maintenance, whereas machining adds recurring operations, fixturing and inspection. A simpler design can reduce both if function is preserved.

Cost Driver Why It Matters Typical Design Question
Side actions or slides Add tooling complexity and maintenance Can the feature follow mold opening direction?
Fragile core pins Increase wear or breakage risk Can the hole be enlarged, shortened or machined later?
Thin tool steel for slots Can reduce tool life Can slot width, depth or radius be adjusted?
Flash-sensitive shutoffs Add finishing and inspection burden Can the parting line move away from critical surfaces?
Secondary machining Adds operation cost but may improve precision Is the feature critical enough to machine?
Inspection requirements Increase quality control workload Which holes or slots are critical dimensions?
Trial mold correction Increases project lead time Can risk be solved during DFM instead?

For two technically acceptable routes, compare fixed tooling and validation costs plus the expected cost per accepted part multiplied by lifetime volume. Include scrap, maintenance and any machining or inspection operations. Higher volume may justify more complex tooling, but no fixed break-even quantity applies. See MIM design for cost.

Feature-Level DFM Checklist Before MIM Tooling

Review each feature individually. Record its drawing feature ID, function, provisional manufacturing route, unresolved risk and required verification. Mark it as provisionally acceptable or requiring engineering review; do not treat this checklist as tooling approval. If tool withdrawal, functional acceptance or inspection access is unresolved, keep the feature open for review.

  • Identify the function of each hole, slot and undercut.
  • Check opening direction and withdrawal interference.
  • Review hole diameter, depth and core support.
  • Review slot width, length and remaining rails.
  • Check internal and external undercut access.
  • Check local wall thickness and weak sections.
  • Identify filling, ejection, debinding and sintering risks.
  • Mark critical dimensions, datums and protected surfaces.
  • Confirm inspection and functional acceptance.
  • Identify machining or sizing requirements.
  • Mark permitted and prohibited design changes.
  • Confirm material, batch size and annual volume.

Prepare for engineering review: supply a 3D STEP model, 2D engineering drawing, material and surface requirements, mating part information, expected loads, critical tolerances, acceptable mark zones, annual quantities and design flexibility. For a complete project review, see DFM for MIM.

Frequently Asked Questions About MIM Holes, Slots and Undercuts

What is the minimum hole diameter for MIM parts?

There is no universal production minimum. PIM International advises avoiding holes below 0.1 mm, but this is not a guaranteed achievable diameter. Depth, pin support, feedstock, tolerance and inspection determine feasibility.

How deep can a blind hole be in MIM?

EPMA gives a general screening recommendation of about twice the core pin diameter. Deeper blind holes require project-specific review of pin deflection, filling and release. This is not an absolute limit.

Do all side holes require mold slides?

No. A suitable parting arrangement or changed orientation may permit direct molding. Otherwise compare side actions, machining and redesign.

How narrow can a slot be in a MIM part?

There is no universal minimum slot width for all MIM geometries. Evaluate the forming blade thickness and height, slot length, material, remaining metal sections and final tolerance.

Can internal undercuts be molded directly in MIM?

Some can be formed using special tooling when there is sufficient access and withdrawal space. Hidden internal bore undercuts are generally best avoided or evaluated for machining or redesign.

Can MIM holes be drilled or reamed after sintering?

Yes, where material, tool access, locating surfaces and machining allowance permit. Drilling or reaming can help achieve critical bore requirements. Reaming alone generally follows the existing hole and should not be relied on to correct substantial location error.

Submit Your Drawing for a Feature-Level DFM Review

If your MIM part includes deep holes, side holes, narrow slots, locking undercuts, cosmetic surfaces near molded features or tight-tolerance assembly details, send your drawing for a feature-level DFM review before tooling.

Please provide 2D drawings, 3D CAD files, material requirements, key tolerances, surface requirements, estimated annual volume and application background. The XTMIM engineering team can review whether your holes, slots and undercuts are suitable for direct MIM molding, require slides or core pins, need secondary machining, or should be redesigned before tooling. This review can help identify flash risk, ejection issues, weak tool steel conditions, sintering distortion and inspection concerns before the project moves into mold manufacturing.

Project-specific design limits

Confirm the proposed feature geometry and manufacturing route with the engineering team before tooling.

Final design limits, tooling feasibility, tolerances and inspection methods depend on the actual material, geometry and production route. Published guidance and hypothetical examples are suitable for preliminary screening.

Technical references

MIMA discusses cored holes, hole orientation, parting planes and complex MIM geometry. MIMA design guidance.

MPIF Standard 35-MIM addresses material specifications for metal injection molded parts. It does not prescribe geometry limits for holes, slots or undercuts. MPIF standards overview.

PIM International discusses common MIM design features and limitations, including holes, slots, grooves and undercuts. PIM International design discussion.

Additional design guidance: EPMA Metal Injection Moulding. Published design recommendations are preliminary references rather than guaranteed XTMIM manufacturing limits.